HOME > ENGLISH HOME > SSS Brand / Product information > Golden Rock/New-type Improved Dental Stone
Golden rock answers to the requests "the high strength","the high fluidity".
1.High strength.
2.High fluidity.Easy to pour.
3.Minimum setting expansion.
4.Hard and smooth surface.
5.Little chipping.
The models such as implant,Konuskrone,attachment,crowns,inlay and bridge.
1. Mixing ratio
100g powder:16 ml water (for the works which needs strength)
100g powder:18 ml water (for the works which needs fluidity)
2. Mixing time : 30 seconds by a mechanical spstulation
3. Pour into an impression without excessive vibration.
4. Remove from the impression after 30 minutes.
And keep in the damp place for 1 hour.
Mixing Ratio | 16% | 18% |
---|---|---|
Setting time | 9min. | 11min. |
Compressive strength | 1h.58.8MPa | 1h.52.4MPa |
dry strength | 147.0MPa | 128.0MPa |
Setting exp.(2h.) | 0.09% | 0.08% |
Reseal after use.
Store in a cool and dry place.
golden brown